| Appearance | | Transparent, no extraneous matter. | | | | | Visual Inspection |
| Density, g/cm3 | | 1.06~ 1.10 | 1.09~ 1.15 | 1.12~ 1.18 | 1.14~ 1.20 | 1.17~ 1.23 | ASTM D792 |
| Curing | Hardness, Shore A | 30±2 | 40±2 | 50±2 | 60±2 | 70±2 | ASTM D2240 |
| Tensile Strength, MPa ≥ | 8.0 | 8.5 | | | | ASTM D412 |
| Elongation at Break, % ≥ | 600 | 500 | 400 | | 300 | |
| Tension Set, % ≤ | 8 | | | | | |
| Tear Strength , Die C kN/m ≥ | 18 | 30 | 35 | | | ASTM D624 |
| Post- curing | Hardness, Shore A | 33±2 | 45±2 | 55±2 | 65±2 | 75±2 | ASTM D2240 |
| Tensile Strength, MPa ≥ | 6.0 | 7.5 | 8.0 | | | ASTM D412 |
| Elongation at Break, % ≥ | 540 | 450 | 350 | 300 | 250 | |
| Tear Strength, Die C kN/m ≥ | 10 | 18 | 20 | | | ASTM D624 |
| Rebound Resilience, % ≥ | | 50 | 45 | | | 40 | / |
| Volume Resistivity, Ω ▪cm ≥ | | 1×10 15 | | | | | IEC 60093 |
| Dielectric Strength, kV/mm ≥ | | 20 | | | | | IEC 60243 |